• Substrate & Cleanliness: Ensure the surface is sound, dry, and free of dirt, oil, and grease. Inadequate cleaning and residual dust will cause Microfino to score and scratch due to coarse aggregates dragged from the Microbase layer.
• Substrate Must Be Level: Microfino is applied in an ultra-thin coat and will not conceal underlying depressions, hollows, or imperfections.
• Working Temperature: Ambient room and substrate temperatures must remain between +10 °C and +25 °C throughout the application.
• Floor Application: Microfino can be applied to small, low-traffic floor areas; however, application on large floor areas is not recommended as the required technique makes uniform installation exceptionally difficult.

1. Application Areas and Tool Selection

Microfino creates a smooth surface with a fine texture and dynamic shading effects. The choice of tool dictates the aesthetic expression (the plastic trowel is the most popular choice):

Plastic Trowel (Most Popular) Most Popular

Produces a softer, calmer, and more homogeneous finish completely free from metallic burnishing marks.

The plastic trowel is by far the most popular choice and is always recommended for white and light shades to keep the finish clean and uniform.
Steel Trowel Marbling

Steel compresses the surface, generating higher movement, contrast, and pronounced marbling effects.

Best suited for darker colors. On light shades, steel trowels can create dark burnish lines if excessive pressure is applied.

2. Preparation and Mixing

Meticulous Cleaning of the Base Coat

The base coat must be sanded completely smooth using 40 grit silicon carbide. Vacuum meticulously and wipe down the surface with a dry microfiber cloth. Inadequate cleaning will cause loose Microbase grains to be dragged across the surface, scratching the thin Microfino layer.

Mixing

Dose Acricem Resin and color pigment into a clean bucket and blend thoroughly. Gradually introduce the Microfino powder while mixing with a mechanical paddle mixer at low speed for at least 4 minutes until a lump-free mortar is achieved. Use the mixing app to calculate material batches based on 10 kg powder.

Pot Life

The mortar has an open pot life of approximately 2–3 hours in the bucket depending on ambient temperature and humidity.

3. Application

Step-by-Step Procedure

1. Perimeter: Start in an upper corner. Work material along the boundaries (approx. 30–40 cm along the ceiling and 50–70 cm downwards). Keep the top face of the trowel blade clean from dried crusts.
2. Distribute: Deposit material along the bottom edge of the freshly applied section.
3. Angle and Scraping Sound: Hold the trowel at an angle of at least 45° with light pressure so only the pores are filled. Listen for the scraping sound—if no scraping sound is heard, the layer is too thick, significantly increasing the risk of air pinholes.
4. Break the Pattern: Immediately rework the wet section with multidirectional, irregular passes to eliminate straight tooling lines and introduce visual movement.
5. Continue & Maintain Wet Edge: Deposit fresh material below the recently applied section (similar to step 1). Next, trowel material along the edge of the initial section. Always maintain a wet edge to ensure seamless blending. When breaking the pattern, feather slightly back over the previously applied surface to integrate old and fresh material invisibly.

Number of Coats

Technically, the system is complete after 1 coat of Microfino. Additional coats are not recommended on floors, as excessive film build reduces surface hardness. If a calmer finish is desired, a second thin coat can be applied identically, or finished with a steel trowel on coat 2 for more pronounced marbling.

💡 Pro Tip for Sharp Internal & External Corners (Final Coat):
To easily execute razor-sharp corners with Microfino, tape off the corners on the 2 adjoining walls before applying the final coat to the active wall. Repeat the process on opposite walls.
• Remove tape immediately after finishing the active wall.
• Position a fan facing the completed walls for accelerated curing.
• Sand and re-tape: After 2–3 hours, sand the corner junctions on the cured walls, mask them, and apply the final coat to the remaining adjacent walls.
This technique works equally well on internal and external corners. While not mandatory, it significantly facilitates a flawless result.

4. Next Steps: Sanding and Sealing

Allow the surface to dry for 24 hours. Sand Microfino lightly using 120 grit silicon carbide on a sander (or 240 grit by hand). Vacuum thoroughly and wipe down the surface with a dry microfiber cloth before sealing begins:

Documents and Technical Datasheets

📄 Technical Documentation: Sttandard Microfino
🛡️ Safety Equipment and Cleaning:
• Protective Equipment: The product contains cement and can cause irritation to skin and eyes. Always wear protective gloves and safety glasses. Use a dust mask/respirator (P2/P3) during powder mixing and all sanding operations. Ensure adequate room ventilation.
• Cleaning: Wash tools immediately with water after use before the mortar sets. For hardened material, clean tools using acetone or cleaning wipes.

How did we do?

TT - Microdeck / Natture M (ENG)

TT - Presealer (ENG)