Skip to main content

TT - Topsealer Pro-Plus (ENG)

Barrier primer that replaces Presealer and gives high protection against stains, liquids and standing water.

tomas martinsson
Updated by tomas martinsson
Guide / Sealing

Pre-treatment: Topsealer Pro-Plus

Barrier primer replacing TT Presealer. Builds an impermeable barrier film offering superior protection against staining, chemicals, and standing water.

🛑 Before You Begin:
‱ Substrate & Cleanliness: Ensure the surface is sound, dry, and free of dirt, oil, and grease.
‱ Working Temperature: Ambient room and substrate temperatures must remain between +10 °C and +25 °C throughout.
‱ Drying Time Prior to Application: Apply Pro-Plus no earlier than 24 hours after the final coat of microcement has dried.
‱ Roller Selection: Always use a 4 mm lint-free mohair roller. Apply very thinly and work the material evenly into the microcement—excessive layer thickness creates an unsightly orange peel texture.

1. Characteristics and Metallic Surfaces

Surface Texture and Color

Pro-Plus builds a heavier protective film than a conventional pre-sealer, which slightly softens the raw tactile feel of the stone while providing an exceptionally resilient barrier. When pigmenting the microcement, follow the dedicated Pro-Plus color recipes, as this product darkens the substrate more than standard primers.

Metallic Surfaces (Pure Mettal)

Outperforms standard sealers on Pure Mettal by preserving the natural metallic brilliance far better than a traditional pre-sealer. However, on purely decorative surfaces subject to no mechanical wear, wax provides the most authentic aesthetic finish.

2. Mixing

🛑 Critical Mixing Precaution – Component B Spills:
It is critical to avoid spilling or splashing Component B onto floor or wall surfaces. The hardener will not cure independently, and microcement applied over contaminated areas will fail to cure properly. Always mix on protective floor covering or in a separate prep area.
Mixing Ratio

For a complete unit, blend 0.8 kg Component A with 0.64 kg Component B. When preparing partial batches, Component A must be stirred meticulously down to the very bottom of the container prior to weighing to redisperse settled solids uniformly. Use the mixing app to calculate precise proportions for smaller batches.

Short Pot Life in Bucket

Usable pot life is only 10–15 minutes after paddle mixing the components together at low speed. Never mix more material than can be applied comfortably within this window. A full kit covers approximately 14 mÂČ.

3. Application and Finishing

Application Technique

Apply in 1 very thin coat using a 4 mm mohair roller. Work the material out thoroughly to achieve an ultra-thin, uniform layer. Drips, ridges, or puddles that cure cannot be sanded away afterward—back-roll the surface meticulously as you progress. Mask adjacent areas carefully to prevent splatter, as cured droplets are virtually impossible to remove.

Drying Time and Intermediate Sanding

Allow Pro-Plus to cure for at least 6 hours. The cured film is completely glossy. Before rolling the topcoat sealer, lightly de-nib the surface by hand using 400 grit sandpaper and wipe away all sanding dust with a dry microfiber cloth.

Documents and Technical Datasheets

📄 Technical Documentation: Topsealer Pro-Plus
đŸ›Ąïž Health & Safety Equipment & Tool Care:
‱ Protective Equipment: Wear nitrile protective gloves and safety glasses during all handling and mixing. Ensure adequate room ventilation during application and curing.
‱ Tool Cleaning: Discard roller sleeves after use. Clean tools and trays immediately with acetone or solvent wipes before the product begins to set.

How did we do?