FC - Forprime EPST (ENG)
Epoxy hybrid for concrete and screed where the mesh is fixed directly to the substrate and troweled in. Mixing, troweling and sand broadcasting.
Updated
by tomas martinsson
Guide / Primer & Base Coat
Forcrete — Forprime EPST
Guide for mixing, troweling, and quartz sand broadcasting of Forprime EPST on concrete and self-leveling screed.
💡 About Forprime EPST:
Forprime EPST is a 2-component epoxy hybrid combining Forprime DPM and Forprime HB/FL. The product is used on concrete and self-leveling screed to eliminate an entire workflow step. Instead of priming first and waiting for full cure before installing mesh and base coat, the reinforcement mesh is installed directly onto the ground substrate. Troweling EPST through the mesh primes the substrate and applies the first base coat in a single combined operation.
Forprime EPST is a 2-component epoxy hybrid combining Forprime DPM and Forprime HB/FL. The product is used on concrete and self-leveling screed to eliminate an entire workflow step. Instead of priming first and waiting for full cure before installing mesh and base coat, the reinforcement mesh is installed directly onto the ground substrate. Troweling EPST through the mesh primes the substrate and applies the first base coat in a single combined operation.
📱 Coverage & Technical Specifications:
• Mixing Ratio (A : B): 75 parts Component A to 25 parts Component B (75 : 25). Always dose using precision scales.
• Sand Addition in Mixture: Add 500 g quartz sand (0.3–0.6 mm) per 1 kg mixed EPST resin. (Example: 750 g A + 250 g B + 500 g sand).
• Material Consumption: Approx. 750 g/m² neat resin when troweling over mesh (total approx. 1.0 kg/m² mixed compound) / approx. 500 g/m² without mesh.
• Surface Sand Broadcast: Broadcast quartz sand directly into the wet resin to complete saturation (approx. 2.5–4 kg/m²).
• Mixing Ratio (A : B): 75 parts Component A to 25 parts Component B (75 : 25). Always dose using precision scales.
• Sand Addition in Mixture: Add 500 g quartz sand (0.3–0.6 mm) per 1 kg mixed EPST resin. (Example: 750 g A + 250 g B + 500 g sand).
• Material Consumption: Approx. 750 g/m² neat resin when troweling over mesh (total approx. 1.0 kg/m² mixed compound) / approx. 500 g/m² without mesh.
• Surface Sand Broadcast: Broadcast quartz sand directly into the wet resin to complete saturation (approx. 2.5–4 kg/m²).
⚠️ Important Information Before Starting:
• Working Temperature: Material, substrate, and ambient air temperatures must remain between +10 °C and +25 °C.
• Substrate Moisture Content: Maximum 4% residual moisture in concrete or self-leveling screed (no surface condensation or standing water film allowed).
• Pot Life in Bucket: Approx. 20–25 minutes at +20 °C. Pour the mixed material immediately onto the floor following mixing to prevent premature exotherm and curing in the bucket.
• Storage: Store frost-free. Shelf life is 12 months in unopened original packaging.
• Working Temperature: Material, substrate, and ambient air temperatures must remain between +10 °C and +25 °C.
• Substrate Moisture Content: Maximum 4% residual moisture in concrete or self-leveling screed (no surface condensation or standing water film allowed).
• Pot Life in Bucket: Approx. 20–25 minutes at +20 °C. Pour the mixed material immediately onto the floor following mixing to prevent premature exotherm and curing in the bucket.
• Storage: Store frost-free. Shelf life is 12 months in unopened original packaging.
1. Substrate Preparation & Reinforcement
1.
Grind the Substrate: Diamond-grind the surface to remove laitance or screed slurry, level out imperfections, and open the substrate pores. Vacuum the surface thoroughly.
2.
Fasten the Mesh: Roll out 160 g fiberglass reinforcement mesh directly onto the cleaned substrate and spot-glue it in place using a hot-melt glue gun. Butt-join the mesh runs edge-to-edge without overlapping to prevent ridges.
2. Step-by-Step Mixing
🛑 Critical Mixing Precaution – Component B Spills:
It is critical to avoid spilling or splashing unmixed Component B onto floor or wall surfaces. It will not cure independently, and microcement applied over contaminated areas will fail to cure properly. Always mix on protective floor covering or in a separate prep area.
It is critical to avoid spilling or splashing unmixed Component B onto floor or wall surfaces. It will not cure independently, and microcement applied over contaminated areas will fail to cure properly. Always mix on protective floor covering or in a separate prep area.
1.
Stir Component A: If using partial units, stir Component A thoroughly down to the bottom of the container before weighing to ensure settled fillers are completely redispersed.
2.
Combine Components A and B: Weigh 75 parts A and 25 parts B into a clean mixing vessel placed on protective floor covering. Stir thoroughly.
3.
Add Sand and Paddle Mix: Add 500 g quartz sand per kilogram of mixed liquid resin. Mix with a mechanical paddle mixer at low speed for at least 3 minutes until the mortar is completely smooth. Pour the mixture immediately onto the floor to prevent premature exotherm in the bucket.
3. Application & Sand Broadcasting
Trowel Application and Quartz Broadcasting
• Application: Pour out the mixed compound and trowel it out very tightly and evenly across the mesh using a steel trowel (consumption approx. 750 g/m² neat resin). Applying a thin layer is critical. Applying thicker layers will not improve coverage; instead, it causes excess sand to pool into mounds, making subsequent diamond grinding significantly harder.
• Sand Broadcasting: Cast an abundant excess of quartz sand directly into the wet resin until the entire surface is completely saturated and no wet resin spots remain visible.
• Curing: Allow to cure for at least 12 hours (overnight).
• Sanding: Sweep up and reclaim excess unbonded sand. Diamond-grind the surface smooth and vacuum thoroughly.
• Sand Broadcasting: Cast an abundant excess of quartz sand directly into the wet resin until the entire surface is completely saturated and no wet resin spots remain visible.
• Curing: Allow to cure for at least 12 hours (overnight).
• Sanding: Sweep up and reclaim excess unbonded sand. Diamond-grind the surface smooth and vacuum thoroughly.
4. Next Steps
Once the surface has been ground and vacuumed, select the next base layer in the system:
Instructions: Apply Forprime HB/FL ↗
Instructions: Apply Microbase XT ↗
Instructions: Application on Screed/Concrete Floors ↗
🛑 Health & Safety Equipment:
• Product contains epoxy resin and may cause skin irritation or allergic reactions.
• Always wear chemical-resistant nitrile gloves during mixing and troweling.
• Wear safety goggles during mechanical paddle mixing.
• Wear an approved particulate respirator during all grinding operations.
• Ensure continuous, adequate workspace ventilation and keep out of reach of children.
• Always wear chemical-resistant nitrile gloves during mixing and troweling.
• Wear safety goggles during mechanical paddle mixing.
• Wear an approved particulate respirator during all grinding operations.
• Ensure continuous, adequate workspace ventilation and keep out of reach of children.
⏱️ Curing & Tool Maintenance (+20 °C):
• Sandable / Grindable: After at least 12 hours.
• Light Traffic: After 2 days.
• Full Cure: After 5 days.
• Tool Cleaning: Clean tools with acetone or solvent wipes immediately after use before the epoxy cures.
• Sandable / Grindable: After at least 12 hours.
• Light Traffic: After 2 days.
• Full Cure: After 5 days.
• Tool Cleaning: Clean tools with acetone or solvent wipes immediately after use before the epoxy cures.
Documents & Technical Datasheets
📄 Technical Documentation: Forcrete Forprime EPST