FC - Forprime DPM (ENG)
Solvent-free two-component epoxy primer used as DPM and bonding bridge. Mixing, application, sand broadcasting and curing times.
Updated
by tomas martinsson
Guide / Epoxy Primer
Forcrete — Forprime DPM
Comprehensive guide for mixing, application, sand broadcasting, and curing times for the 2-component epoxy primer Forprime DPM.
💡 About Forprime DPM:
Forprime DPM is a 2-component, solvent-free epoxy primer that functions as a damp-proof membrane (DPM) and adhesion bonding bridge. It is used on tiled floors, uneven ceramics, vinyl sheeting, worktops, and adjacent to floor drains to ensure superior mechanical keying and create an impermeable, fully moisture-resistant barrier.
Forprime DPM is a 2-component, solvent-free epoxy primer that functions as a damp-proof membrane (DPM) and adhesion bonding bridge. It is used on tiled floors, uneven ceramics, vinyl sheeting, worktops, and adjacent to floor drains to ensure superior mechanical keying and create an impermeable, fully moisture-resistant barrier.
📱 Coverage & Mixing Ratio:
• New DPM (Standard): 78 parts Component A + 22 parts Component B (78:22).
• Previous DPM Formulation: 71 parts Component A + 29 parts Component B (71:29).
(Always verify the batch label on your containers and weigh accurately with a digital scale).
• Material Consumption: Approx. 120–150 g/m².
• Quartz Sand: When broadcasting sand, saturate the surface with quartz sand (grain size 0.1–0.3 mm) directly into the wet resin.
Always use the mixing app to calculate material volumes and exact proportions for your project.
• New DPM (Standard): 78 parts Component A + 22 parts Component B (78:22).
• Previous DPM Formulation: 71 parts Component A + 29 parts Component B (71:29).
(Always verify the batch label on your containers and weigh accurately with a digital scale).
• Material Consumption: Approx. 120–150 g/m².
• Quartz Sand: When broadcasting sand, saturate the surface with quartz sand (grain size 0.1–0.3 mm) directly into the wet resin.
Always use the mixing app to calculate material volumes and exact proportions for your project.
⚠️ Important Information Before Starting:
• Working Temperature: Material, substrate, and ambient air temperatures must remain between +10 °C and +25 °C (maximum 80% relative humidity).
• Residual Moisture: Tolerates up to 6% residual moisture in concrete or screed (ensure no standing liquid or surface condensation is present).
• Thermal Fluctuations: If there is a risk of significant temperature fluctuations, always apply the primer in two coats.
• Storage: Protect from freezing.
• Working Temperature: Material, substrate, and ambient air temperatures must remain between +10 °C and +25 °C (maximum 80% relative humidity).
• Residual Moisture: Tolerates up to 6% residual moisture in concrete or screed (ensure no standing liquid or surface condensation is present).
• Thermal Fluctuations: If there is a risk of significant temperature fluctuations, always apply the primer in two coats.
• Storage: Protect from freezing.
🛑 Critical: Mix a Maximum of 1 kg at a Time!
• Batch Size: Never mix more than 1 kg at a time. The product sets quickly and has a pot life of approximately 20 minutes in the bucket at +20 °C. If you mix too large a volume, you will not have sufficient time to distribute the material before it flashes off, triggering a rapid exothermic reaction with extreme heat buildup.
• Component B Spills: It is critical to avoid spilling or splashing Component B onto floor or wall surfaces. It will not cure independently, and microcement applied over contaminated areas will fail to cure properly. Always mix on protective floor covering or in a separate prep area.
• Temperature Sensitivity: If the product, room, or mixing vessel exceeds +20 °C, open pot life decreases drastically and the resin will accelerate.
• Change Bucket and Roller: If mixing a subsequent batch in the same bucket, or continuing to use the same roller after the pot life has elapsed, uncured epoxy residue will contaminate the new mix, causing it to flash off much faster. Always switch to a clean bucket and fresh roller sleeve.
• Batch Size: Never mix more than 1 kg at a time. The product sets quickly and has a pot life of approximately 20 minutes in the bucket at +20 °C. If you mix too large a volume, you will not have sufficient time to distribute the material before it flashes off, triggering a rapid exothermic reaction with extreme heat buildup.
• Component B Spills: It is critical to avoid spilling or splashing Component B onto floor or wall surfaces. It will not cure independently, and microcement applied over contaminated areas will fail to cure properly. Always mix on protective floor covering or in a separate prep area.
• Temperature Sensitivity: If the product, room, or mixing vessel exceeds +20 °C, open pot life decreases drastically and the resin will accelerate.
• Change Bucket and Roller: If mixing a subsequent batch in the same bucket, or continuing to use the same roller after the pot life has elapsed, uncured epoxy residue will contaminate the new mix, causing it to flash off much faster. Always switch to a clean bucket and fresh roller sleeve.
1. Substrate Preparation
1.
Substrate Inspection: The surface must be sound, dry, and free of dust, dirt, grease, and loose particles.
2.
Grinding & Vacuuming: Diamond-grind tiles to abrade the glazed surface. Vacuum thoroughly so the primer can penetrate and achieve optimal adhesion.
2. Step-by-Step Mixing
1.
Weigh Components: Weigh a maximum of 1 kg total in a clean bucket placed on protective floor covering:
• New DPM: 78 parts Component A to 22 parts Component B (78:22).
• Previous Formulation: 71 parts Component A to 29 parts Component B (71:29).
• New DPM: 78 parts Component A to 22 parts Component B (78:22).
• Previous Formulation: 71 parts Component A to 29 parts Component B (71:29).
2.
Mix: Blend with a mechanical paddle mixer at low speed (approx. 300–400 rpm) for at least 3 minutes.
3.
Dual-Pot Transfer (Critical): Pour the blended epoxy into an entirely new, clean bucket and mix briefly once again. This eliminates any unmixed resin residue clinging to the walls or bottom of the primary container.
3. Application & Sand Broadcasting
Applying the Primer
• Distribution: Pour the mixed epoxy directly onto the substrate. Distribute evenly using a rubber squeegee, smooth trowel, or roller.
• Saturate Pores: Back-roll with a short-pile epoxy roller to ensure complete penetration into all voids and pinholes.
• Sand Broadcasting: Broadcast quartz sand (0.1–0.3 mm) generously into the wet resin until complete saturation is achieved. Sweep and vacuum away all unbonded sand once cured. Sand broadcasting is not required if the substrate is to be covered with Forprime HB or Forprime FL within 24 hours.
• Recoat Window Without Sand: If not broadcasting sand, apply the subsequent layer within 6–24 hours. If more than 24 hours have elapsed, the surface must be abraded to a matte finish using a sander before continuing.
• Saturate Pores: Back-roll with a short-pile epoxy roller to ensure complete penetration into all voids and pinholes.
• Sand Broadcasting: Broadcast quartz sand (0.1–0.3 mm) generously into the wet resin until complete saturation is achieved. Sweep and vacuum away all unbonded sand once cured. Sand broadcasting is not required if the substrate is to be covered with Forprime HB or Forprime FL within 24 hours.
• Recoat Window Without Sand: If not broadcasting sand, apply the subsequent layer within 6–24 hours. If more than 24 hours have elapsed, the surface must be abraded to a matte finish using a sander before continuing.
4. Next Steps
Once Forprime DPM has cured, proceed with the base coat application:
🛑 Health & Safety Equipment:
• Product contains epoxy resin and may cause skin irritation or allergic reactions.
• Always wear approved chemical-resistant nitrile gloves throughout operations.
• Wear safety glasses during mixing to protect against splashes.
• Wear an approved particulate respirator during all sanding operations.
• Ensure continuous, adequate workspace ventilation and keep out of reach of children.
• Always wear approved chemical-resistant nitrile gloves throughout operations.
• Wear safety glasses during mixing to protect against splashes.
• Wear an approved particulate respirator during all sanding operations.
• Ensure continuous, adequate workspace ventilation and keep out of reach of children.
⏱️ Curing Times & Tool Maintenance (+20 °C):
• Foot Traffic: After 5–6 hours.
• Subsequent Coat: After 6 hours.
• Full Cure: After 5 days.
• Tool Cleaning: Clean tools and spills immediately with acetone or solvent wipes before the epoxy cures.
• Foot Traffic: After 5–6 hours.
• Subsequent Coat: After 6 hours.
• Full Cure: After 5 days.
• Tool Cleaning: Clean tools and spills immediately with acetone or solvent wipes before the epoxy cures.
Documents & Technical Datasheets
📄 Technical Documentation: Forcrete Forprime DPM
How did we do?
FC - Forprime EPST (ENG)